[Stephen, Koji]
20 glass beamdumps were bonded at the 40m cleanroom.
Attachment 1: We had 20 fused silica disks with a V-groove and 40 black glass pieces
Attachment 2: The black glass pieces had (usual) foggy features. It is well known to be very stubborn. We had to use IPA/acetone and wiping with pressure. Most of the feature was removed, but we could still see some. We decided to use the better side for the inner V surfaces.
Attachment 3: EP30-2 expiration date was 1/22/2020 👍. 7.66g of EP30-2 was poured and 0.38g of glass sphere was added. Total glue weight was 8.04g
Attachment 4: Glue test piece was baked at 200F in a toaster oven for ~12min. It had no stickiness. It was totally crisp. 👍👍👍
Attachment 5: Painted glue on the V-groove and put the glass pieces in. Then gave a dub of blue at the top and bottom of the V from the outside. In the end, we mostly had the glue went through the V part due to capillary action.
Attachment 6: The 20 BDs were stored in stainless vats. We looked at them for a while to confirm there is no drift and opening of the V part. Because the air bake oven was not available at the time, we decided to leave the assys there for the room temp curing, and then later bake them for the completion of the curing.
|